摘 要:凹土是苏皖地区特色矿产资源,储量丰富且价格低廉。本文以KH-912改性凹土作为吸附剂,考察了吸附剂用量、吸附时间、溶液pH值以及不同温度下不同浓度时,对Pb2+的静态吸附作用。实验结果表明,改性凹土在25 oC时吸附Pb2+的最佳条件为吸附剂用量0.10 g,吸附时间20 min,pH=5.36。拟二级动力学方程能够更好的描述改性凹土对Pb2+的吸附过程。改性凹土能够有效的吸附水溶液中Pb2+,该吸附等温线符合Langmuir吸附等温方程,其在15oC、25oC、35oC时对Pb2+的饱和吸附量分别为77.16 mg/g,78.80 mg/g,80.58 mg/g。54278
毕业论文关键词:改性凹土,Pb2+,吸附
Abstract: Attapulgite is the local characteristics of mineral resources in Anhui and Jiangsu Provinces. This research adopts KH-912 modified attapulgite as adsorbent to study the adsorption properties of Pb2+ from aqueous solution. Batch studies were carried out to investigate various experimental parameters such as adsorbent dosage, contact time and initial pH. The results showed that the optimal conditions for the amount of modified attapulgite adsorption Pb2+ were 0.10 g, the time of 20 min and pH=5.36 at 25 oC. The kinetics of Pb2+ adsorption by modified attapulgite nicely followed the pseudo-second-order kinetics. Adsorption equilibrium data were fitted by the Langmuir isotherm. The maximum adsorption capacity calculated by the Langmuir model was 77.16 mg/g, 78.80mg/g, 80.58 mg/g at 15 °C, 25 °C, and 35 °C, respectively.
Keywords: modified attapulgite, Pb2+, adsorption
目 录
1 前言 3
1.1 重金属离子废水的来源 3
1.2 重金属离子废水的危害 3
1.3 重金属离子废水的处理方法 3
1.4 凹凸棒土的性质 4
1.5 凹凸棒土的改性处理方法及应用现状 4
1.6 本文的研究目的与内容 5
2 实验部分 5
2.1 实验材料 5
2.2 实验仪器和设备 5
2.3 吸附剂的制备 6
2.4 硝酸铅模拟废水的制备 6
2.5 吸附实验 6
3 结果与讨论 7
3.1 改性凹土用量对吸附效果的影响 7
3.2 吸附时间对吸附效果的影响 7
3.3 pH对吸附效果的影响 8
3.4 吸附等温线 9
3.5 吸附动力学 11
结 论 13
参考文献 14
致 谢 16
1 前言
水是万物的生命之源。水不但是体内物质传送的媒介,而且还直接参与生物大分子结构,并共同完成物质代谢、信息代谢和能量代谢,它是自然界和人类生存发展过程中不可缺少的必要因素。然而现在好多水源被重金属污染,铅及其化合物是废水中普遍存在的有毒重金属,它们主要通过消化道和呼吸道进入机体[1],对人类和自然界造成了一定的损失和伤害。
1.1 重金属离子废水的来源
重金属离子废水主要来源于工业废水,如:矿山坑内排水、有色金属冶炼厂除尘排水、有色金属加工厂酸洗水、电镀厂镀件洗涤水[2],以及农药、电解、医药、油漆、烟料、颜料等工业。另外其他废水来源主要是生活污水排放,农田废水和酸雨。